超微粒モリブデン粉末の製造
スポンサーリンク
概要
- 論文の詳細を見る
In order to make fine Mo powder for metallising of ceramic electron tube, we prepared highly voluminous MoO<SUB> 3</SUB> powder by means of oxidation followed by sublimation of Mo filament scrap and then reduced the sublimated MoO<SUB> 3</SUB> to metallic Mo by hydrogen gas.<BR>We found vertical type furnace was suitable for this purpous and the key point of operation was found to prevent the formation of the Mo lower oxide. A good result has been obtained by choosing the furnace temperature of 900-1200°C and treating capacities of 5kgMo/ hr at 1m<SUP>3</SUP>/min air draught ; 7kgMo/hr at 1.4m<SUP>3</SUP>/min were attained, and MoO<SUB> 3</SUB> recovery was kept over 96%.<BR>Sublimated MoO<SUB> 3</SUB> had a purity of 99.9% up and mean particle size of 0.50μ. And the hydrogen-reduced Mo powder indicated its particle size at 0.55μ and proved good result for ceramic use.
- 社団法人 粉体粉末冶金協会の論文