概要
- 論文の詳細を見る
Effects of formalin on tin plating in acidic tin plating bath were studied through measurements of the differential capacity. The addition of 0.3g/l benzalacetone and 5ml/l formalin into the plating bath showed the finest brightening effect. By increasing the additional amount of formalin, the desorption potential on differential capacity-potential curves was shifted to possitive potential, and the potential range which indicated the adsorption was narrowed. Formalin behaved as the assistant of the brightening agent in acidic tin plating.
- 山口大学の論文
著者
関連論文
- 硫酸塩浴からの銅-すず合金めっきに対する浴組成の影響 (分散めっき・合金めっき)
- 酸性スズメッキ浴におけるホルマリン添加の効果と界面微分容量との関係について
- 324 スズメッキ時の光沢剤の浴における吸着挙動について